Single rib tensile strength test
Test equipment: Korea Apparel Testing & Research Institute
     (KATRI)
Standard test method :CRE-type tensile tester
Testing organization: Korea Institute of Construction Technology

Classification
Details
Tester
    United SFM-60 tensile tester
Temperature
     21±2℃
Humidity
     50~70%(Relative humidity)
Tensile velocity
     20±5%/min
Sample width
     20cm(For geogrid samples, more than one-centimeter space was spared from
      the cutting point.)
Number of samples
     6
Tested qualities
     Maximum tensile strength, Tensile stress, Modulus of tensile elasticity,
     Tensile stress curve

※ Results

Classification
TOTOGRID 4T
TOTOGRID 7T
TOTOGRID 10T
Number oftimes tested
Multi-rib tensile strength
(t/m)
Tensile stress
(%)
Multi-rib tensile strength
(t/m)
Tensile stress
(%)
Multi-rib tensile strength
(t/m)
Tensile stress
(%)
1
5.60
6.8
9.21
7.7
11.39
7.3
2
5.61
7.1
9.00
7.6
12.33
7.4
3
5.82
7.4
9.29
7.5
11.93
7.2
4
5.45
7.1
9.29
8.0
11.5.
7.7
5
5.40
7.2
8.80
7.7
12.91
7.9
Average
5.58
7.1
9.12
7.7
12.01
7.5
 
Head office : 1214, Garak-daero, Gangseo-gu, Busan, Republic of Korea       Tel : 070-4827-4066       Fax : 055-346-1724
Branch(factory) : 103-63, Gomo-ro 324beon-gil, Jillye-myeon, Gimhae-si, Gyeongsangnam-do, Republic of Korea       
                          Tel. 82-55-346-1722~3    l   Fax. 82-55-346-1724    l   E-mail. totogrid@naver.com
Copyright(c)2005-2017 TOTOGRID.COM All rights reserved.